1.4 Chemical and mineral admixtures
After this lesson you should be able to:
- Distinguish mineral admixtures (IS 456:2000 cl. 5.2, as amended) from chemical admixtures (cl. 5.5), and state that a chemical admixture, if used, shall comply with IS 9103.
- Name the mineral additions in cl. 5.2.1 and 5.2.2 with the Indian Standards cited after Amendment No. 2, including the usual 5 to 10 percent silica-fume proportion in the amended note to cl. 5.2.1.2, and the metakaoline fineness range in cl. 5.2.1.4.
- Apply the IS 10262:2019 cl. 5.3 water-content adjustment for slump and the usual water-reduction ranges, and the cl. 5.4.1 preliminary-trial increase of cementitious content when fly ash is used, to a numerical proportioning step.
- State the cl. 5.5.3 to 5.5.6 acceptance checks (trial mixes, relative density of each drum, chloride of each batch, and compatibility of two admixtures) and the Table 5 Note 1 rule on counting 5.2 additions in the prescribed cement content.
Theory
An admixture is a material added to a concrete mix, other than the cement, the aggregate and the water, in order to change a fresh or hardened property. Civil practice splits them into two families, and IS 456:2000 treats the two families in two different clauses. Mineral admixtures (also called supplementary cementitious materials) are finely divided inorganic additions — fly ash, ground granulated blast furnace slag, silica fume, metakaoline and rice husk ash — that take part in the cementitious reactions and can replace part of the ordinary Portland cement. Chemical admixtures are typically used at a small fraction of the cement mass and act mainly on the fresh mix: they disperse cement particles, entrain air, accelerate or retard set, or reduce the water needed for a given workability. This lesson is about those two families and the Indian Standard rules that govern them. The cement itself was Lesson 1.1, the aggregates Lesson 1.2 and the mixing water Lesson 1.3. Mix proportioning as a whole is a later chapter.
Cl. 5.2 of IS 456:2000, read with Amendment No. 2 (September 2005), is the mineral-admixture clause. Cl. 5.2.1 allows pozzolanic materials conforming to the relevant Indian Standards to be used with the permission of the engineer-in-charge, provided they are blended uniformly with the cement. After the amendment, fly ash (pulverized fuel ash) used as a part replacement of ordinary Portland cement is to conform to IS 3812 (Part 1), not to the earlier wording “Grade 1 of IS 3812”. Silica fume used as a part replacement of cement is to conform to IS 15388, again with uniform blending; the amended note states that silica fume is usually used in a proportion of 5 to 10 percent of the cement content of a mix. Rice husk ash may be used with the approval of the deciding authority, and only after the particular source has been evaluated for performance and uniformity — the note under cl. 5.2.1.3 warns that a poorly burnt ash can be as harmful as silt, and that water demand and drying shrinkage should be studied first. Metakaoline having a fineness between 700 and 900 m²/kg may be used as a pozzolanic material (cl. 5.2.1.4). Ground granulated blast furnace slag obtained by grinding granulated blast furnace slag conforming to IS 12089 may be used as a part replacement of ordinary Portland cement, again with uniform blending (cl. 5.2.2). Cl. 5.1 also allows other combinations of Portland cement with mineral admixtures of quality conforming to the relevant Indian Standards, provided there are satisfactory data on their suitability, such as a performance test on concrete containing them. Uniform blending is not a slogan: a poorly mixed addition leaves pockets of unreacted powder and pockets of untreated cement, and the member does not have the properties assumed in the mix design.
The prescribed cement content in IS 456:2000 Table 5 is, by Note 1 of that table, irrespective of the grade of cement and is inclusive of the additions mentioned in cl. 5.2. Fly ash or ground granulated blast furnace slag may be taken into account in the concrete composition, with respect to the cement content and the water-cement ratio, if the suitability is established and if the maximum amounts so taken into account do not exceed the limit of pozzolana and slag specified in IS 1489 (Part 1) and IS 455 respectively. That is a durability-table rule, not a licence to ignore trial mixes. IS 10262:2019, the current Indian mix-proportioning guideline (second revision), works in the same direction. Cl. 5.4.1 of that guideline says that when cement is partly replaced by fly ash, ground granulated blast furnace slag, silica fume or other mineral admixtures, an increase in the cementitious materials content may be warranted, particularly if the fly ash is 20 percent or more. The decision may be based on experience and trials, or the cementitious content so calculated may be increased by 10 percent for a preliminary trial, after which the water-cementitious materials ratio is recalculated and checked against IS 456 Table 5. Cl. 5.4.2 leaves the percentage of fly ash or GGBS, for ordinary and standard grades, to the project requirement and the quality of the materials. For high-strength mixes, cl. 6.2.6 and Table 9 give recommended dosage ranges, as a percentage by mass of the total cementitious materials: fly ash 15 to 30, ground granulated blast furnace slag 25 to 50, metakaoline 5 to 15, and silica fume 5 to 10. Those Table 9 figures are for high-strength mixes only; they are not a default for ordinary grades. IS 10262:2019 also names IS 16714:2018 as the specification for ground granulated blast furnace slag in its reference list; IS 456:2000 cl. 5.2.2 names IS 12089. This lesson uses each document’s own citation and does not treat either number as a ranking of the two specifications.
Chemical admixtures are controlled by IS 456:2000 cl. 5.5. If an admixture is used, it shall comply with IS 9103 (cl. 5.5.1); previous experience and data on the material should be considered in relation to the likely standard of supervision and workmanship. Cl. 5.5.2 requires that admixtures should not impair the durability of the concrete, should not combine with the constituents to form harmful compounds, and should not increase the risk of corrosion of the reinforcement. Cl. 5.5.3 requires the workability, the compressive strength and the slump loss of the concrete, with and without the admixture, to be established in trial mixes before the admixture is used. Cl. 5.5.4 requires the relative density of a liquid admixture to be checked for each drum and compared with the specified value before acceptance. Cl. 5.5.5 requires the chloride content of the admixture to be independently tested for each batch before acceptance. Cl. 5.5.6 requires that if two or more admixtures are used in the same mix, data should be obtained on their interaction so that their compatibility can be ensured. A water-reducing admixture and a retarder from two different drums are not “compatible” just because each one separately complies with IS 9103. The total acid-soluble chloride in the concrete at the time of placing, from all constituents including admixtures, is a separate check under cl. 8.2.5.2 and Table 7; that table is not reproduced here, but an accepted admixture can still push the concrete over the Table 7 limit if the other constituents are already salty, which is why cl. 5.5.5 and Table 7 are both needed.
IS 10262:2019 cl. 5.3 gives the mix-proportioning starting point for water. Table 4 of that guideline lists a water content, for a 50 mm slump and saturated-surface-dry aggregate, of 208, 186 and 165 kg per cubic metre for 10 mm, 20 mm and 40 mm nominal maximum size respectively. For a slump other than 50 mm, the water content may be increased or decreased by about 3 percent for each 25 mm of slump, or established by trial. The water so calculated may then be reduced by a chemical admixture conforming to IS 9103: a water-reducing admixture usually decreases the water content by 5 to 10 percent, and a superplasticizing admixture by 20 to 30 percent and above, at appropriate dosages. Annex G of IS 10262:2019 is informative, not a requirement. It describes three ways of using the dispersion: more fluidity at the same water content, a lower water content at the same fluidity, or some of both; it gives typical dose and water-reduction ranges for conventional plasticisers (lignosulphonates or selected carbohydrates: typically 0.3 to 0.5 percent, with 8 to 12 percent water reduction, and noted as suitable to adopt for lower grades) and for superplasticisers (typical dose 0.5 to 1.5 percent, water reduction 15 to 30 percent and more; the three families named are SMFC, SNFC and PCE, with PCE described as used at lower dosages and able to give 30 percent and more water reduction). Cl. 5.3 of the same standard is the figure used in the worked examples when a single percentage has to be chosen from a range; Annex G is cited only as the informative background for those typical doses. EN 934-2, ASTM C494 and ACI 212 are named here for comparison only and are not ranked against IS 9103 or IS 456.
Derivation
- For a change of slump from the 50 mm basis of IS 10262:2019 Table 4, a first estimate of the water content is W_s = W_50 × (1 + 0.03 × Δs / 25 mm), where Δs is the signed slump change in millimetres. The 3 percent per 25 mm figure is the cl. 5.3 guidance; a trial may replace it.
- If a water-reducing or superplasticizing admixture is then used, the reduced water content is W = W_s × (1 − r), where r is the fractional water reduction established for that dosage in the trial (and, as a starting range, 0.05 to 0.10 for a water-reducing admixture or 0.20 to 0.30 and above for a superplasticizing admixture, as in cl. 5.3).
- Without a mineral addition, the cement content is C = W / x, where x is the selected free water-cement ratio. When fly ash (or another mineral addition) is introduced and the cl. 5.4.1 preliminary-trial increase of 10 percent is applied, the cementitious content is C_cm = 1.10 × (W / x). If the fly ash is a fraction f of the cementitious materials, then the fly-ash mass is f C_cm and the Portland-cement mass is (1 − f) C_cm. The water-cementitious materials ratio is then recalculated as W / C_cm and checked against the durability limit that applies to the member.
- A chemical-admixture dosage, when stated as a percentage by mass of cement (or of cementitious materials, if the project so specifies), is m_ad = (d/100) × C. If the admixture is a liquid of relative density ρ_r (dimensionless, relative to water at 1000 kg/m³), the batched volume is V_ad = m_ad / (ρ_r × 1000 kg/m³). Relative density itself is the cl. 5.5.4 acceptance check on each drum; it is not a substitute for a trial dosage.
IS 10262:2019 Table 4 (cl. 5.3), water content for 50 mm slump, SSD aggregate: 208 kg/m³ (10 mm), 186 kg/m³ (20 mm), 165 kg/m³ (40 mm)Slump adjustment (cl. 5.3): about 3 percent water change per 25 mm slump away from 50 mm, or by trialUsual water reduction (cl. 5.3), at appropriate dosages: water-reducing admixture 5 to 10 percent; superplasticizing admixture 20 to 30 percent and abovePreliminary trial with mineral addition (cl. 5.4.1): C_cm may be taken as 1.10 times the cement content calculated from W and the selected water-cement ratio, particularly if fly ash is 20 percent or more; then recalculate W/C_cmSilica fume usual proportion (IS 456:2000 cl. 5.2.1.2 note, as amended): 5 to 10 percent of the cement content of a mixIS 10262:2019 Table 9 (cl. 6.2.6), high-strength mixes only, percent by mass of total cementitious materials: fly ash 15–30; GGBS 25–50; metakaoline 5–15; silica fume 5–10Metakaoline fineness (IS 456:2000 cl. 5.2.1.4): 700 to 900 m²/kg
- The 3 percent per 25 mm slump adjustment, and the 5 to 10 percent and 20 to 30 percent and above water-reduction ranges, are the IS 10262:2019 cl. 5.3 starting guidance. The final water content and the dosage are those established in the trial mixes required by IS 456:2000 cl. 5.5.3.
- Annex G of IS 10262:2019 is informative. Typical dose ranges quoted from it are background, not limits, and are not used as the arithmetic of the worked examples.
- Table 9 dosages apply to high-strength mixes under Section 3 of IS 10262:2019. They are not applied in this lesson to ordinary or standard grades.
- The 10 percent preliminary-trial increase in cl. 5.4.1 is a starting step, not a field mix. The water-cementitious materials ratio must still satisfy IS 456 Table 5 for the exposure, and the amounts of fly ash or slag taken into account must not exceed the limits named in Table 5 Note 1.
- IS 9103, IS 3812 (Part 1), IS 15388, IS 12089, IS 1489 (Part 1), IS 455 and IS 16714 are named as cited. Their internal tables are not used, because those official texts were not on the box at writing.
- Uniform blending, drum-by-drum relative density, batch-by-batch chloride, and compatibility of combined admixtures are acceptance conditions, not optional extras.
- This lesson does not proportion a project mix, does not reproduce Table 4, Table 5, Table 7 or Table 9 as figures, and does not rank IS, EN or ASTM provisions.
Codes and standards
Indian Standards are cited by number and clause only; no clause text, tables or figures are reproduced. Other standards are listed for comparison, not ranked.
- IS 456:2000 cl. 5.1 and 5.2–5.2.2, with Amendment No. 2 (September 2005) to cl. 5.2.1.1 (IS 3812 (Part 1)) and cl. 5.2.1.2 (IS 15388, and the usual 5 to 10 percent silica-fume note), including cl. 5.2.1.3 rice husk ash, cl. 5.2.1.4 metakaoline, and cl. 5.2.2 GGBS (IS 12089).
- IS 456:2000 cl. 5.5.1–5.5.6 — compliance with IS 9103; durability and corrosion; trial mixes of workability, strength and slump loss; relative density of each drum; chloride of each batch; compatibility of two or more admixtures.
- IS 456:2000 Table 5 Note 1 — prescribed cement content inclusive of cl. 5.2 additions; fly ash and GGBS may be taken into account subject to suitability and to the pozzolana and slag limits of IS 1489 (Part 1) and IS 455. Cl. 8.2.5.2 and Table 7 — total acid-soluble chloride in the concrete, named but not reproduced.
- IS 10262:2019 cl. 5.3 and Table 4; cl. 5.4.1–5.4.2; cl. 6.2.6 and Table 9 (high-strength mixes); Annex G (informative). IS 9103 is the chemical-admixture specification named by both IS 456 and IS 10262.
- EN 934-2, ASTM C494 and ACI 212 are named for comparison only, not ranked.
Worked examples
Problem. A trial mix is being proportioned for a 20 mm nominal maximum size of aggregate and a 100 mm slump, using a superplasticizing admixture conforming to IS 9103. Starting from IS 10262:2019 Table 4 (186 kg/m³ of water at 50 mm slump, SSD aggregate) and the cl. 5.3 guidance of about 3 percent water change per 25 mm of slump, estimate the water content after the slump adjustment. Then reduce that water by 20 percent, a value chosen inside the cl. 5.3 usual range of 20 to 30 percent and above for a superplasticizing admixture. Report both water contents in kg/m³. Say, in one sentence, what still has to be established before the admixture is used on the pour.
- The slump increase from the 50 mm Table 4 basis is 50 mm, which is 2 × 25 mm, so the cl. 5.3 adjustment is about 2 × 3 percent = 6 percent.
- Water after the slump adjustment W_s = 186 × 1.06 = 197.16 kg/m³.
- With a 20 percent superplasticizer reduction, W = 197.16 × (1 − 0.20) = 197.16 × 0.80 = 157.728 kg/m³, or 157.7 kg/m³ to one decimal place.
- IS 456:2000 cl. 5.5.3 still requires the workability, compressive strength and slump loss, with and without the admixture, to be established in trial mixes before the admixture is used. The 157.7 kg/m³ figure is a cl. 5.3 starting estimate, not a field batch weight.
Answer. W_s = 197.16 kg/m³ after the slump adjustment; W = 157.7 kg/m³ after a 20 percent reduction. Trial mixes under cl. 5.5.3 are still required before use.
Problem. An ordinary-grade trial uses 20 mm aggregate, a 50 mm slump and no slump adjustment, so the Table 4 water content is 186 kg/m³. The selected free water-cement ratio, before any mineral addition, is 0.45 (a stipulated value, not a copied Table 5 entry). Fly ash is to be 25 percent of the total cementitious materials. Apply the IS 10262:2019 cl. 5.4.1 option of increasing the calculated cement content by 10 percent for a preliminary trial (the fly ash is more than 20 percent). Find the cementitious content, the fly-ash and Portland-cement masses, and the recalculated water-cementitious materials ratio.
- Cement content before the addition C = 186 / 0.45 = 413.33 kg/m³.
- Preliminary-trial cementitious content C_cm = 1.10 × 413.33 = 454.67 kg/m³.
- Fly ash = 0.25 × 454.67 = 113.67 kg/m³. Portland cement = 0.75 × 454.67 = 341.00 kg/m³.
- Recalculated water-cementitious materials ratio W / C_cm = 186 / 454.67 = 0.409.
- This 0.409 ratio, and the fly-ash amount taken into account, must still be checked against IS 456 Table 5 for the exposure, and against Table 5 Note 1 (the fly ash taken into account must not exceed the pozzolana limit of IS 1489 (Part 1), and suitability must be established). The 10 percent increase is a preliminary-trial step, not the finished field mix.
Answer. C_cm = 454.67 kg/m³, fly ash 113.67 kg/m³, Portland cement 341.00 kg/m³, W/C_cm = 0.409, still to be checked against Table 5 and Note 1.
Step-by-step procedure
- Decide whether a mineral addition, a chemical admixture, or both, will be used, and why (workability, water reduction, heat, durability, or a specified cementitious system).
- For a mineral addition, use only a material that conforms to the standard named in IS 456:2000 cl. 5.2 as amended (IS 3812 (Part 1) for fly ash, IS 15388 for silica fume, IS 12089 for GGBS as cited there, and the stated fineness for metakaoline), and arrange uniform blending with the cement. Rice husk ash needs a source evaluation and the deciding authority’s approval.
- Select a free water-cement or water-cementitious materials ratio that will satisfy IS 456 Table 5 for the exposure. If fly ash or GGBS is to be counted in the cement content, apply Table 5 Note 1, including the IS 1489 (Part 1) and IS 455 quantity limits.
- Start the water content from IS 10262:2019 Table 4, adjust about 3 percent per 25 mm of slump if the slump is not 50 mm, or set it by trial, and then apply a water reduction only if a chemical admixture conforming to IS 9103 is used, with the reduction taken from a value inside the cl. 5.3 range and confirmed in trials.
- If fly ash is 20 percent or more, consider the cl. 5.4.1 10 percent preliminary-trial increase in cementitious content and recalculate W/C_cm.
- Before accepting a chemical admixture: confirm IS 9103 compliance (cl. 5.5.1); run trial mixes for workability, strength and slump loss (cl. 5.5.3); check the relative density of each drum (cl. 5.5.4); test the chloride of each batch (cl. 5.5.5); and, if two or more admixtures are combined, obtain compatibility data (cl. 5.5.6). Check the total chloride of the concrete against cl. 8.2.5.2 and Table 7.
- Do not take a Table 9 (high-strength) dosage as the default for an ordinary-grade mix. Confirm the field batch against the trial, including slump loss with time and temperature.
Site notes
- A mineral addition that is “added in the hopper” but not blended uniformly will show itself as colour bands, variable slump and erratic 28-day results. Follow the blending method used in the successful trial.
- Liquid admixture dispensers drift. Cl. 5.5.4 is a drum check of relative density, not a calibration of the pump; check both.
- Do not make up a missed dosage by pouring an unmeasured second shot at the pump. Re-dose only in the way the trial allowed, and record it.
- Two admixtures in one mix — a superplasticizer and a retarder, for example — need a compatibility record (cl. 5.5.6), not just two separate IS 9103 certificates.
- A “chloride-free” label on a drum is not the cl. 5.5.5 batch test, and it is not the Table 7 check on the concrete as placed.
- In hot weather the slump loss with a given dosage can be much faster than in the laboratory trial. Cl. 5.5.3 asks for slump loss to be established; repeat the look on a warm afternoon before a long haul.
- Silica fume at the usual 5 to 10 percent of cement is very fine and raises water demand if it is not used with a suitable superplasticizer. That is one reason cl. 5.5.3 and the IS 10262 note on increased water or admixture demand with a high mineral dosage both matter.
- Using a chemical admixture that has not been shown to comply with IS 9103, or skipping the trial mixes of cl. 5.5.3 because “we always use 0.8 percent”.
- Taking the IS 10262:2019 Table 9 high-strength dosage ranges as if they applied to ordinary or standard grades, or treating Annex G typical doses as mandatory limits.
- Counting fly ash or GGBS in the Table 5 cement content without the suitability check and without respecting the IS 1489 (Part 1) or IS 455 quantity limits in Table 5 Note 1.
- Forgetting to recalculate the water-cementitious materials ratio after a cl. 5.4.1 increase in cementitious content, or applying the 10 percent increase when it has not been chosen as a preliminary-trial step.
- Checking the relative density of one drum and assuming the next drum is the same, or accepting a chloride figure from a previous batch (cl. 5.5.4 and 5.5.5 are per drum and per batch).
- Combining two admixtures without compatibility data (cl. 5.5.6), or assuming that a low chloride in the admixture automatically satisfies Table 7 for the concrete.
- Ranking IS 9103 against EN 934-2 or ASTM C494, or substituting an overseas dosage table for the Indian trial.
Mineral additions: IS 456 cl. 5.2 as amended (fly ash IS 3812 (Part 1); silica fume IS 15388, usually 5–10 percent of cement; GGBS IS 12089; metakaoline 700–900 m²/kg); blend uniformly. Chemical: comply with IS 9103; trial workability, strength and slump loss; RD each drum; chloride each batch; check compatibility if two are combined. IS 10262:2019 Table 4 water, about 3 percent per 25 mm slump; WR 5–10 percent, SP 20–30 percent and above, then confirm by trial.
Summary
- Mineral admixtures under IS 456:2000 cl. 5.2 (as amended in 2005) are part replacements of Portland cement and must conform to the named Indian Standards and be blended uniformly with the cement.
- Silica fume is usually used at 5 to 10 percent of the cement content; metakaoline is used at a fineness of 700 to 900 m²/kg. Table 5 Note 1 allows fly ash and GGBS to be counted in the prescribed cement content only within stated limits and if suitability is established.
- Chemical admixtures, if used, shall comply with IS 9103. Trial mixes must establish workability, strength and slump loss; each drum’s relative density and each batch’s chloride must be checked; two admixtures in one mix need a compatibility check.
- IS 10262:2019 cl. 5.3 gives starting water contents, a slump adjustment of about 3 percent per 25 mm, and usual water-reduction ranges of 5 to 10 percent (water-reducing) and 20 to 30 percent and above (superplasticizing). Table 9 dosage ranges are for high-strength mixes only.
- A proportioning estimate is not a field mix until the trials and the durability and chloride checks have been satisfied.
Practice questions
Tap a question to see the answer.
1Which Indian Standard must a chemical admixture comply with, under IS 456:2000 cl. 5.5.1?
IS 9103.
2After Amendment No. 2, which standard does fly ash used under cl. 5.2.1.1 have to conform to?
IS 3812 (Part 1).
3What usual silica-fume proportion is given in the amended note to cl. 5.2.1.2?
5 to 10 percent of the cement content of a mix.
4A 20 mm mix starts from the Table 4 water of 186 kg/m³ at 50 mm slump. A water-reducing admixture is used at a 10 percent reduction, with no slump change. What is the reduced water content?
W = 186 × 0.90 = 167.4 kg/m³.
5A high-strength trial has a total cementitious content of 500 kg/m³ and uses silica fume at 8 percent of that total, a value inside IS 10262:2019 Table 9. What are the silica-fume and the remaining cementitious masses?
Silica fume = 0.08 × 500 = 40 kg/m³; remaining cementitious material = 460 kg/m³. Table 9 applies to high-strength mixes only.
6Two liquid admixtures are to be used in the same mix, each with its own IS 9103 certificate. What extra requirement does cl. 5.5.6 set?
Data should be obtained on their interaction so that their compatibility can be ensured. Separate certificates are not, by themselves, that data.
References
Standard texts, listed in no order of merit. Our explanations, examples and diagrams are original; nothing is copied from these books.
- A. M. Neville, Properties of Concrete, Pearson, 5th edition, 2011.
- P. K. Mehta, P. J. M. Monteiro, Concrete: Microstructure, Properties, and Materials, McGraw Hill, 4th edition, 2014.
- IS 456:2000 cl. 5.2 (as amended by Amendment No. 2, September 2005) and cl. 5.5–5.5.6, cited by number only. IS 10262:2019 cl. 5.3, 5.4.1–5.4.2, 6.2.6 and Annex G (informative), cited by clause and table number only. ISO / ASTM / ACI documents named for comparison only.