1.2 Aggregates
After this lesson you should be able to:
- Distinguish fine aggregate from coarse aggregate at the 4.75 mm IS sieve, and name the main types of natural and manufactured aggregate in IS 383:2016.
- State the IS 456:2000 cl. 5.3 rules that limit the nominal maximum size of coarse aggregate, including the tighter rule for heavily reinforced ribs in cl. 5.3.3.1, and apply them to a member.
- Compute the fineness modulus of a fine aggregate from a sieve analysis, and carry out a moisture correction between stockpile and saturated-surface-dry batch masses.
- Name the principal quality limits that IS 383:2016 places on deleterious material, particle shape, and mechanical properties, citing the clause, not a copied table.
Theory
Aggregate occupies most of the volume of ordinary concrete. It is not an inert filler: its size, grading, shape, strength, absorption and impurities affect workability, the water demand, elastic stiffness, shrinkage and durability. This lesson is about those particles and the Indian Standard rules that govern them. Mixing water is Lesson 1.3; admixtures are Lesson 1.4; how the paste binds the aggregate was Lesson 1.1.
IS 383:2016 cl. 3.1 defines fine aggregate as aggregate most of which passes the 4.75 mm IS sieve, with only so much coarser material as the grading clause permits. Cl. 3.2 defines coarse aggregate as aggregate most of which is retained on that same sieve. All-in-aggregate (cl. 3.3) is a combined fine-and-coarse material; IS 456:2000 cl. 5.3.4 requires coarse and fine aggregate to be batched separately, and allows all-in-aggregate only where the engineer-in-charge specifically permits it.
Fine aggregate may be natural (uncrushed) sand, crushed stone sand, crushed gravel sand, mixed sand (a blend of natural and crushed sand), or manufactured fine aggregate produced from other than natural sources (IS 383 cl. 3.1.1–3.1.4). Coarse aggregate may be uncrushed, crushed, partially crushed, or manufactured (cl. 3.2, including the note). IS 456:2000 cl. 5.3 requires aggregates to comply with IS 383, and says that as far as possible preference shall be given to natural aggregates. Manufactured aggregates, including recycled concrete aggregate (RCA) and recycled aggregate (RA), are permitted only to the extents in IS 383 Table 1 (as amended in August 2017). They shall not be used in prestressed concrete (cl. 4.2.2). After Amendment 1, bottom ash from thermal power plants is listed as a fine-aggregate option for lean concrete (less than M 15) only, at a maximum of 25 percent, and is not for plain or reinforced concrete. In any one structure, only one type of manufactured coarse aggregate and one type of manufactured fine aggregate shall be used (Table 1, Note 2).
IS 456:2000 cl. 5.3.3 deals with size. The nominal maximum size of coarse aggregate should be as large as possible within the limits specified, but in no case greater than one-fourth of the minimum thickness of the member, provided the concrete can still be placed so as to surround all reinforcement and fill the corners of the form. For most work, 20 mm aggregate is suitable. Where there is no restriction to the flow of concrete into the section, 40 mm or a larger size may be permitted. In thin sections, closely spaced reinforcement or small cover, consideration should be given to 10 mm nominal maximum size. Plums above 160 mm may be used in plain concrete, up to 20 percent by volume, only when specifically permitted; they shall be distributed evenly and shall be not closer than 150 mm from the surface. For heavily reinforced concrete members, as in the ribs of main beams, cl. 5.3.3.1 usually restricts the nominal maximum size to 5 mm less than the minimum clear distance between the main bars, or 5 mm less than the minimum cover, whichever is smaller.
Grading is the particle-size distribution. IS 383:2016 Table 7 gives the permitted passing percentages for single-sized and graded coarse aggregates in the usual nominal sizes, including 10 mm, 20 mm and 40 mm. Table 9 gives four grading zones for fine aggregate, Zones I to IV, from coarser to finer. A fine aggregate that complies with any zone may be used in concrete, but as the grading becomes finer (Zone I towards Zone IV) the fine-to-coarse ratio should be reduced (Notes 2 and 3). Note 4 recommends that Zone IV fine aggregate should not be used in reinforced concrete unless tests have shown that the proposed mix is suitable. For crushed stone sand, the permitted passing on the 150 µm sieve is increased to 20 percent (Note 1); for the other zones the 150 µm passing limit is 10 percent in Zones I to III and 15 percent in Zone IV. On the 4.75 mm sieve, Zones I to III require 90 to 100 percent passing, and Zone IV requires 95 to 100 percent; all four zones require 100 percent passing the 10 mm sieve. A convenient textbook index, the fineness modulus, is the sum of the cumulative percentages retained on the standard series 4.75, 2.36, 1.18, 0.600, 0.300 and 0.150 mm sieves, divided by 100. It is not an IS 383 acceptance limit; it is used here only as a labelled working index (Neville).
Quality is more than grading. IS 383:2016 cl. 5.1 requires aggregates to be hard, strong, dense, durable and free from injurious amounts of disintegrated pieces, alkali, vegetable matter and other deleterious substances. Table 2 (cl. 5.2.1) limits individual deleterious substances and their total (except mica). Among the figures that are clearly stated: material finer than the 75 µm IS sieve shall not exceed 3.00 percent by mass for uncrushed fine aggregate, 15.00 percent for crushed sand, 12.00 percent for mixed sand and 10.00 percent for manufactured fine aggregate, and 1.00 percent for coarse aggregate of each type, when tested as in IS 2386 (Part 1). Note 3 of Table 2 deals with mica in fine aggregate: where no strength and durability tests are conducted, mica may be limited to 1.00 percent by mass; where tests ensure adequate performance, muscovite may be permitted up to 3.00 percent, or muscovite plus biotite up to 5.00 percent, subject to a total of deleterious materials including mica of 8.00 percent for uncrushed fine aggregate and 5.00 percent for crushed or mixed sand. Combined flakiness and elongation index, determined in that order on the same sample as in cl. 5.3 and IS 2386 (Part 1), shall not exceed 40 percent for uncrushed or crushed aggregate, unless the engineer-in-charge relaxes the limit on the basis of performance.
Mechanical properties are in cl. 5.4, tested as in IS 2386 (Part 4). For concrete for wearing surfaces (the clause lists runways, roads, pavements, tunnel linings that carry water, spillways and stilling basins), the aggregate crushing value and the aggregate impact value shall not exceed 30 percent, and the Los Angeles abrasion value shall not exceed 30 percent. For concrete other than for wearing surfaces, the impact value shall not exceed 45 percent and the abrasion value shall not exceed 50 percent; if the crushing value exceeds 30 percent, the ten-percent-fines test should be conducted and the minimum load for ten percent fines should be 50 kN. A note to cl. 5.4.2 states that for concrete of grades M 65 and above the maximum crushing value and impact value shall not exceed 22 percent. Soundness (cl. 5.5) matters where frost is expected; alkali-aggregate reaction (cl. 5.6) can damage concrete only when a high moisture level, a source of alkali, and a susceptible aggregate are present together. Other aggregates such as slag or crushed overburnt brick or tile may be used for plain concrete under IS 456 cl. 5.3.1 if they are suitable in strength and durability, contain not more than 0.5 percent sulphates as SO3, and do not absorb more than 10 percent of their own mass of water.
Stockpile moisture must be brought back to the saturated-surface-dry (SSD) basis used in mix design. Absorption is the moisture held in the pores at the SSD condition, expressed on the oven-dry mass; free (surface) moisture is the difference between the total moisture of the stockpile and the absorption, also on the oven-dry mass. The wet mass to batch in order to supply a required SSD mass is (SSD mass) × (1 + total moisture) / (1 + absorption). The free water in that wet mass must be deducted from the mix water (or added, if the stockpile is drier than SSD). These are mass-balance definitions used with IS 2386 (Part 3); they are not a substitute for a site-specific moisture measurement.
Derivation
- Fine and coarse aggregate are separated, for the purpose of the standard, at the 4.75 mm IS sieve, as defined in IS 383:2016 cl. 3.1 and 3.2.
- The one-fourth-thickness rule is a direct comparison: d_max ≤ t_min / 4, together with the placing proviso in IS 456 cl. 5.3.3 and the usual preferred sizes 20 mm, 40 mm and 10 mm named in that clause.
- For a heavily reinforced rib, cl. 5.3.3.1 gives d_max usually ≤ min(s_clear − 5 mm, c_min − 5 mm), where s_clear is the minimum clear distance between main bars and c_min is the minimum cover. The smaller of those two values governs, and the nominal size chosen is the standard size that does not exceed it.
- Fineness modulus FM = (Σ cumulative percent retained on the 4.75, 2.36, 1.18, 0.600, 0.300 and 0.150 mm sieves) / 100. It is a textbook working index, not an IS 383 limit.
- Let w_tot be the total moisture and w_abs the absorption, both as fractions of the oven-dry mass. The oven-dry mass in a required SSD mass M_ssd is M_od = M_ssd / (1 + w_abs). The wet mass to batch is M_wet = M_od (1 + w_tot) = M_ssd (1 + w_tot) / (1 + w_abs). The free water in that wet mass is M_free = M_od (w_tot − w_abs) = M_wet − M_ssd, which is deducted from the mix water when w_tot > w_abs.
Fine / coarse split: 4.75 mm IS sieve (IS 383:2016 cl. 3.1 and 3.2)d_max ≤ t_min / 4 (IS 456:2000 cl. 5.3.3), with the placing proviso in that clauseFor a heavily reinforced rib: d_max usually ≤ min(s_clear − 5 mm, c_min − 5 mm) (cl. 5.3.3.1)FM = (Σ cumulative % retained on 4.75, 2.36, 1.18, 0.600, 0.300, 0.150 mm) / 100 (textbook index)M_wet = M_ssd (1 + w_tot) / (1 + w_abs); M_free = M_wet − M_ssdCombined flakiness and elongation index ≤ 40 percent, unless relaxed (IS 383:2016 cl. 5.3)Wearing-surface crushing, impact and abrasion values: 30 percent maximum (IS 383:2016 cl. 5.4)
- The 4.75 mm split and the grading zones follow IS 383:2016, including Amendment 1 (2017). A project specification may cite an earlier edition; the edition named in the specification governs.
- The one-fourth-thickness and 5 mm-less rules are necessary conditions from IS 456 cl. 5.3.3 and 5.3.3.1. They do not, by themselves, choose a size if placing or pumping needs a smaller size.
- Cl. 5.3.3.1 is stated for heavily reinforced members such as the ribs of main beams. It is not automatically applied to every slab or wall in this lesson.
- Fineness modulus is a textbook working index. It is not a pass/fail limit in IS 383.
- Moisture corrections use moisture and absorption expressed on the oven-dry mass. A site moisture meter must be used with the same definition.
- Mechanical-property limits depend on whether the concrete is for a wearing surface and on the grade (the 22 percent note for M 65 and above). The clause list of wearing-surface uses is not extended in this lesson.
- This lesson does not select an aggregate source for a project, and it does not reproduce IS 383 tables.
Codes and standards
Indian Standards are cited by number and clause only; no clause text, tables or figures are reproduced. Other standards are listed for comparison, not ranked.
- IS 456:2000 cl. 5.3 — aggregates shall comply with IS 383; preference, as far as possible, to natural aggregates. Cl. 5.3.1 (slag, crushed overburnt brick or tile in plain concrete: sulphate as SO3 not more than 0.5 percent; absorption not more than 10 percent). Cl. 5.3.2 (heavyweight or lightweight aggregates). Cl. 5.3.3 and 5.3.3.1 (nominal maximum size, including plums). Cl. 5.3.4 (separate batching; all-in-aggregate only if specifically permitted).
- IS 383:2016 (third revision) with Amendment 1 (August 2017) — definitions cl. 3.1–3.3; manufactured aggregates Table 1 as amended, and cl. 4.2.2 (not for prestressed concrete); quality cl. 5.1; deleterious materials Table 2 and cl. 5.2.1; combined flakiness and elongation index cl. 5.3 (40 percent); mechanical properties cl. 5.4; soundness cl. 5.5; alkali-aggregate reaction cl. 5.6; grading Tables 7, 9 and 10.
- IS 2386 (Parts 1 to 8):1963 — methods of test, cited by part (particle size and shape; deleterious materials; specific gravity, density, voids, absorption and bulking; mechanical properties; and so on). Sampling: IS 2430.
- EN 12620 (aggregates for concrete) and ASTM C33 are named for comparison only, not ranked.
Worked examples
Problem. A heavily reinforced beam rib has a minimum thickness of 300 mm, a minimum cover of 25 mm, and a minimum clear distance between main bars of 18 mm. Using IS 456:2000 cl. 5.3.3 and cl. 5.3.3.1, what nominal maximum size of coarse aggregate should be considered? State every limit you use.
- One-fourth of the minimum thickness is 300 / 4 = 75 mm. Cl. 5.3.3 therefore does not, by itself, forbid 40 mm or 20 mm on thickness grounds, and it names 20 mm as suitable for most work.
- The member is a heavily reinforced rib, so cl. 5.3.3.1 applies. Five millimetres less than the minimum clear distance between main bars is 18 − 5 = 13 mm. Five millimetres less than the minimum cover is 25 − 5 = 20 mm. The smaller value is 13 mm.
- The usual nominal sizes that do not exceed 13 mm include 10 mm. A 20 mm nominal size would exceed 13 mm and should not be used in this rib under cl. 5.3.3.1.
- The placing proviso of cl. 5.3.3 still applies: the concrete must be able to surround the bars and fill the form. If a 10 mm mix cannot be placed, the detailing or the mix must be changed; the size is not increased past the 13 mm restriction.
Answer. Consider a 10 mm nominal maximum size. The governing limit is cl. 5.3.3.1: min(13 mm, 20 mm) = 13 mm.
Problem. A 500 g oven-dry sample of uncrushed fine aggregate is sieved on the standard fine-aggregate series. Masses retained are: 4.75 mm, 10 g; 2.36 mm, 50 g; 1.18 mm, 80 g; 0.600 mm, 120 g; 0.300 mm, 140 g; 0.150 mm, 70 g; pan, 30 g. (a) Check the 10 mm (all of the sample is smaller than 10 mm), 4.75 mm and 150 µm passing against the IS 383:2016 Table 9 limits quoted in the lesson for Zones I to III, and compute the fineness modulus. (b) The mix asks for 650 kg of this sand on an SSD basis. A stockpile measurement gives a total moisture of 4.0 percent and an absorption of 1.0 percent, both on the oven-dry mass. What wet mass should be batched, and how much free water does that wet mass contain?
- Sum of retained masses = 10 + 50 + 80 + 120 + 140 + 70 + 30 = 500 g, so the percentages are on a 500 g base.
- Cumulative masses retained: 10, 60, 140, 260, 400 and 470 g on the six standard sieves, and 500 g including the pan. Cumulative percentages retained: 2.0, 12.0, 28.0, 52.0, 80.0 and 94.0 percent.
- Percent passing: 10 mm, 100 percent (within the 100 percent Table 9 figure for every zone); 4.75 mm, 100 − 2.0 = 98.0 percent (within 90 to 100 percent for Zones I to III); 150 µm, 100 − 94.0 = 6.0 percent (within 0 to 10 percent for Zones I to III, uncrushed). The 150 µm crushed-sand allowance of 20 percent is not needed here.
- Fineness modulus FM = (2.0 + 12.0 + 28.0 + 52.0 + 80.0 + 94.0) / 100 = 268.0 / 100 = 2.68. This is a textbook index, not an IS 383 limit.
- Wet mass to batch: M_wet = 650 × (1 + 0.040) / (1 + 0.010) = 650 × 1.04 / 1.01 = 669.3 kg.
- Free water in that wet mass: M_free = 669.3 − 650 = 19.3 kg. Equivalently, oven-dry mass = 650 / 1.01 = 643.56 kg and free water = 643.56 × (0.040 − 0.010) = 19.3 kg. That 19.3 kg must be deducted from the mix water.
Answer. Passing checks for the quoted Table 9 limits are satisfied; FM = 2.68 (textbook index). Batch 669.3 kg of wet sand and deduct 19.3 kg of free water from the mix water.
Step-by-step procedure
- Identify whether the material is being used as fine aggregate, coarse aggregate, or all-in-aggregate, using the 4.75 mm IS sieve and IS 383 cl. 3.1–3.3. Batch coarse and fine separately unless all-in-aggregate is specifically permitted (IS 456 cl. 5.3.4).
- Choose a nominal maximum size from IS 456 cl. 5.3.3 and, if the member is a heavily reinforced rib, cl. 5.3.3.1. Write t_min / 4, s_clear − 5 mm and c_min − 5 mm, and take the governing (smallest applicable) value.
- Obtain a grading by IS 2386 (Part 1) and compare it with IS 383 Table 7 (coarse) or Table 9 (fine). For fine aggregate, record the zone and apply the crushed-sand and Zone IV notes where they matter. Compute a fineness modulus only as a working index, if asked.
- Check quality: deleterious materials (Table 2, including the 75 µm and mica notes), combined flakiness and elongation index (cl. 5.3, 40 percent), and the relevant crushing, impact or abrasion limit in cl. 5.4, using IS 2386 tests.
- If a manufactured aggregate is proposed, apply Table 1 as amended and cl. 4.2.2 (not for prestressed concrete), and keep the final grading within Tables 7 to 9 (Table 1, Note 4).
- Measure stockpile moisture and absorption on the oven-dry basis, convert the SSD batch mass to a wet mass, and adjust the mix water by the free water.
- Do not use a copied table as a site ticket; use the official standard named in the specification.
Site notes
- Ask for the current test certificates (grading, 75 µm fines, shape index, crushing or impact, and, where relevant, soundness or alkali reactivity) for each source and each nominal size, and match them to the specification edition of IS 383.
- Do not use a 20 mm stockpile in a congested beam rib that cl. 5.3.3.1 has limited to 10 mm. Segregated stockpiles of mixed sizes are not a 20 mm graded aggregate.
- Keep coarse and fine in separate bins. All-in-aggregate from a single heap is permitted only if the engineer-in-charge has specifically allowed it.
- Rain on a sand heap changes free moisture quickly. Remeasure moisture when batching, and deduct (or add) the free water. Do not guess.
- Crushed sand often carries more material finer than 75 µm than river sand. That is permitted up to the Table 2 limit (15 percent for crushed sand) but it changes water demand; it is not “the same sand with a different name”.
- Recycled and slag aggregates have stated maximum replacements and are not for prestressed concrete under IS 383 cl. 4.2.2. Do not substitute them for natural aggregate without those checks.
- Taking “20 mm is suitable for most work” as a permission to use 20 mm in a congested rib, ignoring cl. 5.3.3.1.
- Using one-fourth of the span, or of the overall depth including finish, instead of one-fourth of the minimum thickness of the member.
- Treating all-in-aggregate as a substitute for separately batched fine and coarse aggregate without specific permission (cl. 5.3.4).
- Using the 20 percent passing-150 µm allowance for crushed stone sand as if it applied to uncrushed sand, or using Zone IV sand in reinforced concrete without the tests required by Table 9 Note 4.
- Treating fineness modulus as an IS 383 pass/fail limit, or computing it on a non-standard sieve set.
- Forgetting to deduct free moisture from the mix water, so the true water-cement ratio rises and the intended paste structure (Lesson 1.1) is lost.
- Using a manufactured or recycled aggregate in prestressed concrete, or above the Table 1 (amended) replacement limits.
- Ranking IS 383 against EN 12620 or ASTM C33, or treating an overseas grading as a substitute for the IS 383 zone.
Fine / coarse split at 4.75 mm (IS 383). d_max ≤ t_min/4, and for a heavy rib usually ≤ min(s_clear, c_min) − 5 mm (IS 456 cl. 5.3.3 and 5.3.3.1). Combined shape index ≤ 40 percent; wearing-surface crushing/impact/abrasion ≤ 30 percent (IS 383 cl. 5.3–5.4). M_wet = M_ssd (1+w_tot)/(1+w_abs).
Summary
- Fine aggregate mostly passes the 4.75 mm IS sieve; coarse aggregate is mostly retained on it. IS 456 requires compliance with IS 383 and, as far as possible, prefers natural aggregates.
- Nominal maximum size is limited by one-fourth of the minimum thickness and, in heavily reinforced ribs, by 5 mm less than the clear bar spacing or the cover, whichever is smaller. 20 mm suits most work; 10 mm is often needed in thin or congested sections.
- IS 383:2016 Table 9 defines four fine-aggregate grading zones; Table 7 covers coarse sizes. Fineness modulus is a textbook index, not a code limit.
- Deleterious materials, a combined flakiness and elongation index of 40 percent, and the cl. 5.4 crushing, impact and abrasion limits protect strength and durability. Manufactured aggregates have stated replacement limits and are not for prestressed concrete.
- Batch by the SSD mass and correct for stockpile moisture, or the true water-cement ratio will not be the one that was designed.
Practice questions
Tap a question to see the answer.
1At which IS sieve do IS 383:2016 cl. 3.1 and 3.2 split fine aggregate from coarse aggregate?
The 4.75 mm IS sieve.
2A wall is 160 mm thick. What is the cl. 5.3.3 one-fourth-thickness limit on nominal maximum aggregate size?
160 / 4 = 40 mm.
3A beam rib has a minimum cover of 20 mm and a minimum clear spacing of 14 mm. What is the cl. 5.3.3.1 limit?
min(14 − 5, 20 − 5) = min(9, 15) = 9 mm, so a 10 mm nominal size would exceed it; the detailing or the cover/spacing must be consistent with the size that is actually used.
4Cumulative percentages retained on the 4.75, 2.36, 1.18, 0.600, 0.300 and 0.150 mm sieves are 0, 8, 22, 48, 78 and 95. What is the fineness modulus?
FM = (0+8+22+48+78+95)/100 = 2.51.
5A mix needs 500 kg of SSD sand. Total moisture is 5.0 percent and absorption is 1.0 percent, both on oven-dry mass. What wet mass should be batched, and what free water does it contain?
M_wet = 500 × 1.05 / 1.01 = 519.8 kg; free water = 519.8 − 500 = 19.8 kg.
6What combined flakiness and elongation index shall not be exceeded for uncrushed or crushed aggregate under IS 383:2016 cl. 5.3, unless the engineer-in-charge relaxes it?
40 percent.
References
Standard texts, listed in no order of merit. Our explanations, examples and diagrams are original; nothing is copied from these books.
- A. M. Neville, Properties of Concrete, Pearson, 5th edition, 2011.
- P. K. Mehta, P. J. M. Monteiro, Concrete: Microstructure, Properties, and Materials, McGraw Hill, 4th edition, 2014.
- IS 456:2000 cl. 5.3–5.3.4, cited by number only. IS 383:2016 (third revision) with Amendment 1 (August 2017), cited by clause and table number only.