1.1 Cement hydration and microstructure
After this lesson you should be able to:
- Describe, in outline, how Portland cement clinker compounds react with water to form a hardened paste, and name the main hydration products.
- Explain how leftover mixing water becomes capillary pores, and why a lower water-cement ratio, once the paste can still be compacted, leads to a denser microstructure.
- Use a stated textbook figure for chemically combined water at complete hydration (0.23 by mass of cement) to estimate leftover water or a degree of hydration in an illustrative calculation.
- Name the types of cement that IS 456:2000 cl. 5.1 permits, by their IS numbers, and state that the type must be appropriate for the intended use.
Theory
Cement is the hydraulic binder in concrete. When it is mixed with water it first forms a plastic paste and then, through a set of chemical reactions called hydration, a rigid, porous solid that binds the aggregate. This lesson is about that reaction and the microstructure it leaves behind. Aggregates, mixing water quality, and admixtures are the following lessons; mix design and strength come later.
Ordinary Portland cement is made by heating a designed mixture of calcareous and argillaceous materials to form clinker, then grinding the clinker with a little gypsum. The clinker is a combination of four main compounds, written in cement chemists’ notation as C3S (alite), C2S (belite), C3A (aluminate) and C4AF (ferrite). C stands for CaO, S for SiO2, A for Al2O3 and F for Fe2O3. Gypsum is added to control the otherwise rapid reaction of C3A. The proportions of these compounds vary with the cement; they are not a single set of numbers in IS 456, and they are not guessed in this lesson.
On contact with water, C3S and C2S form a poorly crystalline calcium silicate hydrate, usually written C-S-H, and calcium hydroxide, CH (portlandite). C-S-H is the main source of strength in the paste. C3A, with gypsum, forms ettringite (an AFt phase) at early ages and later other aluminate hydrates. C3S reacts relatively quickly and contributes much of the early strength and early heat. C2S reacts more slowly and contributes more to later strength. C3A reacts rapidly and can produce a large early heat if it is not controlled by gypsum. These are qualitative comparisons, not a ranking of cements for a project.
Hydration is exothermic and is not instantaneous. A thin layer of hydrate forms on the grain, a dormant period follows, and then the reaction accelerates and later slows as ions must diffuse through the growing hydrate layer. Unhydrated cores can remain inside larger grains for a long time, especially at low water-cement ratios. The degree of hydration, α, is the fraction of the cement that has reacted. It increases with time, with temperature, and with the availability of water, and it is lower if the paste dries out (which is why curing matters; Lesson 2.4).
The microstructure of a hardened paste is a mixture of C-S-H gel, CH crystals, other hydrates, unhydrated cement, and pores. Two pore families are useful in a first picture. Gel pores are an intrinsic part of the C-S-H and are very small. Capillary pores are the leftover spaces that were filled by mixing water that has not been chemically combined, together with any volume change of the reaction. A convenient textbook working figure, due to Powers and used in standard texts such as Neville, is that complete hydration of Portland cement chemically combines about 0.23 of the cement mass as non-evaporable water, and that a further amount of water is associated with the gel. That 0.23 figure is not a clause of IS 456 and is used here only as a labelled working value. If the mixing water-cement ratio is higher than the water that can be combined, the excess remains as capillary water and, when it is lost or remains as a free-water-filled space, as capillary porosity. A lower water-cement ratio, provided the concrete can still be placed and compacted, therefore leaves fewer capillary pores and a denser paste. This is the microstructural reason behind Abrams’ law, which is treated with strength in Chapter 3.
IS 456:2000 cl. 5.1 requires that the cement used shall be one of the types listed there, and that the type selected shall be appropriate for the intended use. In our own words, the list includes 33, 43 and 53 grade ordinary Portland cement, conforming respectively to IS 269, IS 8112 and IS 12269 (as printed in IS 456:2000; IS 269:2015 now covers all three OPC grades in one standard); rapid-hardening Portland cement (IS 8041); Portland slag cement (IS 455); Portland pozzolana cement, fly-ash based (IS 1489 Part 1) and calcined-clay based (IS 1489 Part 2); hydrophobic cement (IS 8043); low-heat Portland cement (IS 12600); and sulphate-resisting Portland cement (IS 12330). Mineral admixtures used with cement are treated in cl. 5.2 (for example fly ash conforming to IS 3812, used as a part replacement of ordinary Portland cement when uniform blending is ensured). Other families of cement, such as those in EN 197 or ASTM C150, are named only so that a reader can find the comparable documents; they are not ranked against the Indian Standards.
Hydration and microstructure set the scene for everything that follows: workability is the behaviour of the fresh paste and concrete, strength and durability are the behaviour of the hardened pore structure, and mix design is the choice of water-cement ratio and paste content that makes that pore structure possible on site. A cement type that is appropriate for the exposure (for example a slag or sulphate-resisting cement in a sulphate environment) is a materials choice under cl. 5.1, not a substitute for a correctly proportioned and cured concrete.
Derivation
- Write the water-cement ratio by mass as w/c = Mw / Mc, where Mc is the mass of cement and Mw is the mass of mixing water.
- At a degree of hydration α, take the chemically combined (non-evaporable) water as wn = α wn,∞ Mc, where wn,∞ is a stated working value for complete hydration. In the illustrative examples, wn,∞ = 0.23 (Powers / Neville-type figure, not an IS 456 clause).
- The leftover mixing water is then Mw − wn = Mc [ w/c − α wn,∞ ]. For complete hydration (α = 1) this leftover is Mc (w/c − 0.23), provided w/c is not less than 0.23.
- If that leftover water is taken to occupy volume (Mw − wn) / ρw, with ρw = 1000 kg/m³ in the examples, that volume is an upper-bound picture of the capillary water space associated with leftover mixing water. It is not a complete model of capillary porosity (it omits chemical shrinkage and gel water); it is used only to make the mass balance numerical.
- Equivalently, if a laboratory measures a non-evaporable water content wn,meas per unit mass of cement, an estimated degree of hydration is α = wn,meas / wn,∞, using the same stated wn,∞.
w/c = Mw / Mc (mass ratio, dimensionless)wn = α wn,∞ Mc (kg); illustrative working value wn,∞ = 0.23Leftover mixing water ≈ Mc (w/c − α wn,∞) (kg), for w/c ≥ α wn,∞α ≈ wn,meas / wn,∞ (illustrative estimate)ρw = 1000 kg/m³ in the worked examplesThe 0.23 figure is a textbook working value for chemically combined water at complete hydration, not a code limit
- The 0.23 combined-water figure is a conventional textbook working value for Portland cement at complete hydration. It is not exact for every cement, and it is not an IS 456 requirement. Examples that use it are labelled illustrative.
- The leftover-water volume uses ρw = 1000 kg/m³ and ignores chemical shrinkage and gel water. It is a teaching mass balance, not a pore-structure model for design.
- Degree of hydration estimated as wn,meas / wn,∞ assumes that the measured non-evaporable water corresponds to the same definition as wn,∞.
- Qualitative statements about the relative speed of C3S, C2S and C3A are for ordinary Portland cements at ordinary temperatures. They are not a specification of any one commercial cement.
- IS 456 cl. 5.1 lists permitted types; the actual cement used on a project must match the specification and be appropriate for the intended use. This lesson does not select a cement for a site.
- Blended cements and mineral admixtures change the later hydrate assemblage and the heat of hydration; they are introduced here only as types named in cl. 5.1 and 5.2, and are treated more fully in Lesson 1.4.
Codes and standards
Indian Standards are cited by number and clause only; no clause text, tables or figures are reproduced. Other standards are listed for comparison, not ranked.
- IS 456:2000 cl. 5.1 — cement: the cement shall be one of the listed types and the type shall be appropriate for the intended use. Types and their IS numbers, in our words: 33 / 43 / 53 grade OPC (IS 269, IS 8112, IS 12269); rapid-hardening Portland (IS 8041); Portland slag (IS 455); PPC fly-ash based (IS 1489 Part 1); PPC calcined-clay based (IS 1489 Part 2); hydrophobic (IS 8043); low-heat Portland (IS 12600); sulphate-resisting Portland (IS 12330).
- IS 456:2000 cl. 5.2 — mineral admixtures, including fly ash conforming to IS 3812 used as part replacement of ordinary Portland cement when uniform blending is ensured.
- The 0.23 combined-water working value is not an IS 456 clause. It is a textbook / Powers-type figure used only in illustrative examples.
- EN 197 (common cements) and ASTM C150 / C1157 are named for comparison only, not ranked.
Worked examples
Problem. A batch uses 400 kg of Portland cement and 180 kg of mixing water. (a) What is the water-cement ratio? (b) Taking the textbook working value wn,∞ = 0.23, how much water is chemically combined if hydration is complete, and how much mixing water is left over? (c) Taking ρw = 1000 kg/m³, what volume does that leftover water occupy? State the limits of this picture.
- Water-cement ratio w/c = 180 / 400 = 0.45.
- Combined water at complete hydration wn = 0.23 × 400 = 92 kg.
- Leftover mixing water = 180 − 92 = 88 kg.
- Volume of that leftover water = 88 / 1000 = 0.088 m³.
- This 0.088 m³ is a mass-balance picture of leftover mixing water. It is not a complete estimate of capillary porosity, because it omits chemical shrinkage and water held in the gel, and because complete hydration may not be reached in a real paste at this water-cement ratio.
- The figure 0.23 is a textbook working value, not a requirement of IS 456.
Answer. w/c = 0.45; combined water 92 kg; leftover 88 kg, occupying 0.088 m³ in this mass-balance picture.
Problem. A laboratory reports a non-evaporable water content of 0.15 g per gram of Portland cement in a paste. Taking the same working value wn,∞ = 0.23, estimate the degree of hydration. If the paste was mixed at w/c = 0.40, estimate the leftover mixing water per kilogram of cement.
- Estimated degree of hydration α = 0.15 / 0.23 = 0.652, or 65.2 %.
- Combined water per kilogram of cement = 0.15 kg (the measured value).
- Mixing water per kilogram of cement = 0.40 kg.
- Leftover mixing water per kilogram of cement = 0.40 − 0.15 = 0.25 kg, or 250 g.
- The estimate of α is only as good as the working value wn,∞ and the definition of non-evaporable water used in the test. It is not a code acceptance limit.
Answer. α ≈ 65.2 %; leftover mixing water ≈ 0.25 kg per kg of cement.
Step-by-step procedure
- From the mix, write Mc and Mw and compute w/c = Mw / Mc.
- If a degree of hydration or a combined-water working value is to be used, write it down and label it as a textbook working value, not as a code limit.
- Compute combined water wn = α wn,∞ Mc and leftover water Mw − wn, and, if asked, a leftover volume with a stated ρw.
- If a measured non-evaporable water is given, estimate α = wn,meas / wn,∞ and state the assumption.
- When choosing or checking a cement type against a specification, use IS 456 cl. 5.1 (and cl. 5.2 if a mineral admixture is used) and the product’s own IS number. Do not choose a type from this lesson alone.
- Keep qualitative statements about C3S, C2S and C3A separate from any numerical mass balance.
Site notes
- Cement must be stored dry. A bag that has already set in lumps has begun to hydrate and should not be used as fresh cement.
- The type of cement on the bag (OPC grade, PPC, slag, sulphate-resisting, and so on) should match what the specification asked for under IS 456 cl. 5.1.
- A low water-cement ratio improves the paste only if the concrete is still fully compacted. Adding extra water on site to make placing easier increases capillary space and undoes the intended microstructure.
- Heat of hydration matters in large pours: a low-heat cement (IS 12600) or a suitable blended cement may be specified, together with placing and curing measures. Cement type alone does not control thermal cracking.
- Early drying stops hydration. Keep the paste moist for the specified curing period so that α can increase and capillary space can fill with hydrate.
- Treating the 0.23 combined-water figure as an IS 456 limit, or as exact for every cement.
- Thinking that a water-cement ratio below 0.23 means there is no capillary porosity; unhydrated cement and chemical shrinkage still leave a pore structure, and complete hydration may not occur.
- Adding water on site and then expecting the designed microstructure and strength.
- Using 53-grade OPC where a slag, pozzolana or sulphate-resisting cement was specified, or the reverse, without regard to cl. 5.1 “appropriate for the intended use”.
- Confusing the grade of OPC (33, 43, 53) with the grade of concrete (M20, M25, …). They are different numbers, in different standards.
- Assuming all of the mixing water disappears into hydrates. Much of it remains as leftover water and becomes capillary pores.
- Ranking Indian and overseas cement standards, or treating EN 197 or ASTM C150 as a substitute for the IS listed in cl. 5.1.
w/c = Mw/Mc. Illustrative combined-water working value at complete hydration: about 0.23 by mass of cement (textbook, not IS 456). Leftover water ≈ Mc(w/c − α×0.23). IS 456 cl. 5.1: use a listed cement type appropriate for the intended use.
Summary
- Portland cement hydrates with water to form C-S-H (the main binder), calcium hydroxide and other hydrates, leaving unhydrated cores and pores.
- C3S reacts relatively quickly, C2S more slowly; C3A is rapid and is controlled by gypsum. These are qualitative statements.
- Leftover mixing water becomes capillary space. A lower water-cement ratio, if the concrete can still be compacted and is cured, gives a denser paste.
- A textbook working value for chemically combined water at complete hydration is about 0.23 by mass of cement; it is not a code clause.
- IS 456:2000 cl. 5.1 lists permitted cement types by their IS numbers and requires the type to be appropriate for the intended use. Mineral admixtures are in cl. 5.2.
Practice questions
Tap a question to see the answer.
1Name the two main products of the hydration of C3S and C2S.
Calcium silicate hydrate (C-S-H) and calcium hydroxide (CH, portlandite).
2A mix has 350 kg cement and 140 kg water. What is w/c?
w/c = 140/350 = 0.40.
3Using wn,∞ = 0.23 and α = 1, how much combined water is estimated for 350 kg of cement?
0.23 × 350 = 80.5 kg.
4For that mix, how much mixing water is left over at complete hydration on this working model?
140 − 80.5 = 59.5 kg.
5A paste has wn,meas = 0.184 g/g and wn,∞ = 0.23. Estimate α.
α = 0.184/0.23 = 0.800, or 80.0 %.
6Which IS 456 clause lists permitted cement types, and which IS number is named there for 43-grade ordinary Portland cement?
Clause 5.1; IS 8112.
References
Standard texts, listed in no order of merit. Our explanations, examples and diagrams are original; nothing is copied from these books.
- A. M. Neville, Properties of Concrete, Pearson, 5th edition, 2011.
- P. K. Mehta, P. J. M. Monteiro, Concrete: Microstructure, Properties, and Materials, McGraw Hill, 4th edition, 2014.
- IS 456:2000, Plain and Reinforced Concrete — Code of Practice, Bureau of Indian Standards (clauses 5.1 and 5.2 cited by number only).